Electrical Conductivity and Resistivity for Titanium and Titanium Alloys
Material |
Conductivity |
Resistivity |
Reference |
Notes |
|
(% IACS) | (Siemens/m) | (Ohm-m) | (See Below) | ||
Titanium |
|||||
Titanium | 3.10 | 1.798E+06 | 5.562E-07 | ECTM | |
Titanium | 2.20 | 1.276E+06 | 7.837E-07 | CSNDT | |
ASTM grades 1, 2, 3, 4, 7, and 11 | 3.3-4.1 | 4.2E-7--5.2E-7 | MHASM2 | conductivity converted from resistivity | |
Ti-5Al-2.5Sn | 1.10 | 1.570E-06 | MHASM2 | conductivity converted from resistivity | |
Ti-5Al-2.5Sn (low O2) | 0.96 | 1.800E-06 | MHASM2 | conductivity converted from resistivity | |
Ti-8Al-1Mo-1V | 0.87 | 1.990E-06 | MHASM2 | conductivity converted from resistivity | |
Ti-11Sn-1Mo2.25Al-5.0Zr-1Mo-0.2Si | 1.06 | 1.620E-06 | MHASM2 | conductivity converted from resistivity | |
Ti-6Al-2Sn-4Zr-2Mo | 0.91 | 1.900E-06 | MHASM2 | conductivity converted from resistivity | |
IMI 685 | 1.03 | 1.680E-06 | MHASM2 | conductivity converted from resistivity | |
Ti-8Mn | 1.87 | 9.200E-07 | MHASM2 | conductivity converted from resistivity | |
Ti-6Al-4V | 1.01 | 1.710E-06 | MHASM2 | conductivity converted from resistivity | |
Ti-6AL-4V | 1.00 | 5.800E+05 | 1.724E-06 | ECTM | |
Ti-6Al-6V-2Sn | 1.10 | 1.570E-06 | MHASM2 | conductivity converted from resistivity | |
Ti-7Al-4Mo | 1.01 | 1.700E-06 | MHASM2 | conductivity converted from resistivity | |
IMI 550 | 1.09 | 1.580E-06 | MHASM2 | conductivity converted from resistivity | |
Ti-11.5Mo-Zr-4.5Sn | 1.11 | 1.560E-06 | MHASM2 | conductivity converted from resistivity | |
Ti-15V-3Cr-3Al-3Sn | 1.17 | 1.470E-06 | MHASM2 | conductivity converted from resistivity |
- CSNDT=CSNDT compiled by Eddy Current Technology Incorporated
- ECTM=Eddy Current Testing Manual on Eddy Current Method compiled by Eddy Current Technology Incorporated MHASM2=ASM Metals Handbook--Volume 2, Tenth Edition