Electrical Conductivity and Resistivity for Magnesium and Magnesium Alloys

Material

Conductivity

Resistivity

Reference

Notes

(% IACS) (Siemens/m) (Ohm-m) (See Below)

Magnesium Alloys (Wrought)

AZ10A 26.94
6.400E-08 MHASM2 conductivity converted from resistivity
AZ31B, AZ31C 18.50
9.200E-08 MHASM2
AZ61A 11.60
1.250E-07 MHASM2
AZ80A 10.60
1.450E-07 MHASM2
HK31A-H24 28.26
6.100E-08 MHASM2 conductivity converted from resistivity
HK31A-O 28.74
6.000E-08 MHASM2 conductivity converted from resistivity
HM21A-H24 33.16
5.200E-08 MHASM2 conductivity converted from resistivity
HM21A-O 34.48
5.000E-08 MHASM2 conductivity converted from resistivity
HM31A-F 26.00
6.600E-08 MHASM2
M1A 34.50
5.000E-08 MHASM2
ZC71 31.93
5.400E-08 MHASM2 conductivity converted from resistivity
ZK60A-F 29.00
5.945E-08 MHASM2 resistivity converted from conductivity
ZK60A-T5 30.00
5.747E-08 MHASM2 resistivity converted from conductivity
                  

Magnesium Alloys (Cast)

Pure 38.60 2.239E+07 4.467E-08 CSNDT
Magnesium Alloys (Cast) 15.00 8.700E+06 1.149E-07 CSNDT
AZ80BTA 10.80 6.264E+06 1.596E-07 CSNDT
Magnesium Cast Alloys 9.00 5.220E+06 1.916E-07 CSNDT
A2 80 14.60 8.468E+06 1.181E-07 CSNDT
A231 17.20 9.976E+06 1.002E-07 CSNDT
A251 12.80 7.424E+06 1.347E-07 CSNDT
A261 12.30 7.134E+06 1.402E-07 CSNDT
T454 12.50 7.250E+06 1.379E-07 CSNDT
AM100A-F 11.50
1.500E-07 MHASM2
AM100A-T4 9.90
1.750E-07 MHASM2
AM110A-T6 12.30
1.400E-07 MHASM2
AZ63A-F 15.00
1.150E-07 MHASM2
AZ63A-T4 12.30
1.400E-07 MHASM2
AZ63A-T5 13.80
1.250E-07 MHASM2
AZ81A 12.00
1.300E-08 MHASM2
AZ91A-F 10.10
1.700E-07 MHASM2
AZ91C-F, AZ91E-F 11.50
1.500E-07 MHASM2
AZ91C-T4, AZ91E-T4 9.90
1.750E-07 MHASM2
AZ91C-T6, AZ91E-T6 11.20
1.515E-07 MHASM2
AZ92A-F 12.30
1.400E-07 MHASM2
AZ92A-T4 10.50
1.650E-07 MHASM2
AZ92A-T6 12.30
1.400E-07 MHASM2
EQ21 25.20
6.850E-08 MHASM2
EZ33A 25.00
7.000E-08 MHASM2
HK31A-T6 22.00
7.700E-08 MHASM2
HK31A-H24 28.26
6.100E-08 MHASM2 conductivity converted from resistivity
HK31A-O 28.74
6.000E-08 MHASM2 conductivity converted from resistivity
HZ32A 26.50
9.500E-08 MHASM2
K1A 30.25
5.700E-08 MHASM2 conductivity converted from resistivity
QE22A 25.20
6.850E-08 MHASM2
QH21A 25.17
6.850E-08 MHASM2 conductivity converted from resistivity
WE43 11.65 6.800E+06 1.480E-07 MHASM2 conductivity (IACS) converted from resistivity
WE54 9.97 5.800E+06 1.730E-07 MHASM2 conductivity (IACS) converted from resistivity
ZC63 31.93
5.400E-08 MHASM2 conductivity converted from resistivity
ZE41A-T5 28.74
6.000E-08 MHASM2 conductivity converted from resistivity
ZE63A 30.90
5.600E-08 MHASM2
ZH62A 26.50
6.500E-08 MHASM2
ZK51A 28.00
6.200E-08 MHASM2
  • CSNDT=CSNDT compiled by Eddy Current Technology Incorporated
  • MHASM2=ASM Metals Handbook--Volume 2, Tenth Edition

Compiled by the Collaboration for NDT Education.