Electrical Conductivity and Resistivity for Aluminum and Aluminum Alloys
Material |
Conductivity |
Resistivity |
Reference |
Notes |
|
(% IACS)
|
(Siemens/m)
|
(Ohm-m)
|
(See Below)
|
||
Aluminum |
|||||
Pure |
61.00
|
3.538E+07
|
2.826E-08
|
ECTM
|
|
99.99% |
64.94
|
3.767E+07
|
2.655E-08
|
CSNDT
|
|
99.99% |
64.94
|
3.767E+07
|
2.655E-08
|
ALASM
|
|
Red X-8 Cond. Stress Relieved |
29.00
|
1.682E+07
|
5.945E-08
|
CSNDT
|
|
Red X-8 As Cast |
26.00
|
1.508E+07
|
6.631E-08
|
CSNDT
|
|
11S Cond. T3 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
13 |
39.00
|
2.262E+07
|
4.421E-08
|
CSNDT
|
|
14S Cond. "0" |
50.00
|
2.900E+07
|
3.448E-08
|
CSNDT
|
|
14S Cond. T6 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
17S Cond. "0" |
45.00
|
2.610E+07
|
3.831E-08
|
CSNDT
|
|
17S Cond. T4 |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
18S Cond. "0" |
50.00
|
2.900E+07
|
3.448E-08
|
CSNDT
|
|
18S Cond. T61 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
2S Cond. "0" |
59.00
|
3.422E+07
|
2.922E-08
|
CSNDT
|
|
2S Cond. H18 |
57.00
|
3.306E+07
|
3.025E-08
|
CSNDT
|
|
24S Cond. "0" |
50.00
|
2.900E+07
|
3.448E-08
|
CSNDT
|
|
24S Cond. T4 |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
24S Cond. T6 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
3S Cond. "0" |
50.00
|
2.900E+07
|
3.448E-08
|
CSNDT
|
|
3S Cond. H 12 |
42.00
|
2.436E+07
|
4.105E-08
|
CSNDT
|
|
3S Cond. H 14 |
41.00
|
2.378E+07
|
4.205E-08
|
CSNDT
|
|
3S Cond. H 18 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
32S Cond. "0" |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
32S Cond. T6 |
35.00
|
2.030E+07
|
4.926E-08
|
CSNDT
|
|
40E |
35.00
|
2.030E+07
|
4.926E-08
|
CSNDT
|
|
43 (Annealed) |
42.00
|
2.436E+07
|
4.105E-08
|
CSNDT
|
|
43 As Cast |
37.00
|
2.146E+07
|
4.660E-08
|
CSNDT
|
|
A51S Cond. "0" |
55.00
|
3.190E+07
|
3.135E-08
|
CSNDT
|
|
A51S Cond. T4 and T6 |
45.00
|
2.610E+07
|
3.831E-08
|
CSNDT
|
|
52S Cond. "0" and H 38 |
35.00
|
2.030E+07
|
4.926E-08
|
CSNDT
|
|
53S Cond. "0" |
45.00
|
2.610E+07
|
3.831E-08
|
CSNDT
|
|
53S Cond. T4 and T6 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
56S Cond. "0" |
29.00
|
1.682E+07
|
5.945E-08
|
CSNDT
|
|
56S Cond. H 38 |
27.00
|
1.566E+07
|
6.386E-08
|
CSNDT
|
|
61S Cond. "0" |
45.00
|
2.610E+07
|
3.831E-08
|
CSNDT
|
|
61S Cond. T4 and T6 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
75S Cond. T6 |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
85 |
28.00
|
1.624E+07
|
6.158E-08
|
CSNDT
|
|
|
|||||
Aluminum Allcast |
|||||
As Cast |
27.00
|
1.566E+07
|
6.386E-08
|
CSNDT
|
|
Cond. Sol. H.T. & Stress Relieved |
36.00
|
2.088E+07
|
4.789E-08
|
CSNDT
|
|
Sol H.T. and Aged |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
Stress Relieved |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
|
|
|
|
||
Aluminum Alloy (Wrought) |
|
||||
1050-0 |
61.30
|
2.810E-08
|
ALASM
|
||
1060-O |
62.00
|
2.780E-08
|
ALASM
|
||
1060-H18 |
61.00
|
2.780E-08
|
ALASM
|
||
1100 |
57.00 - 61.80
|
3.445E+07
|
2.903E-08
|
NDT Mag
|
|
1100-O |
59.00
|
2.920E-08
|
ALASM
|
||
1100-H18 |
57.00
|
3.020E-08
|
ALASM
|
||
1145-O |
61.00
|
2.830E-08
|
ALASM
|
||
1145-H18 |
60.00
|
2.830E-08
|
ALASM
|
||
1199-O |
64.50
|
2.670E-08
|
ALASM
|
||
1350-O |
61.80
|
2.790E-08
|
ALASM
|
||
1350-Hx |
61.00
|
2.820E-08
|
ALASM
|
||
2011-T3 |
36.00 - 36.50
|
2.103E+07
|
4.756E-08
|
NDT Mag
|
|
2011-T3 and T4 |
39.00
|
4.400E-08
|
ALASM
|
||
2011-T8 |
45.00
|
3.800E-08
|
ALASM
|
||
2014-F and -0 |
48.60 - 50.70
|
2.880E+07
|
3.473E-08
|
NDT Mag
|
|
2014-O |
50.00
|
3.400E-08
|
ALASM
|
||
2014-T3 and -T4 |
32.50 - 34.80
|
1.952E+07
|
5.124E-08
|
NDT Mag
|
|
2014-T3, T4, and T451 |
34.00
|
5.100E-08
|
ALASM
|
||
2014-T6 |
38.00 - 39.70
|
2.253E+07
|
4.438E-08
|
NDT Mag
|
|
2014-T6, T651, and T652 |
40.00
|
4.300E-08
|
ALASM
|
||
2017-F |
49.30 - 49.50
|
2.865E+07
|
3.490E-08
|
NDT Mag
|
|
2017-O |
50.00
|
3.500E-08
|
ALASM
|
||
2017-T4 |
34.00
|
5.000E-08
|
ALASM
|
||
2024-F |
46.80 - 48.50
|
2.764E+07
|
3.618E-08
|
NDT Mag
|
|
2024-O |
50.00
|
3.400E-08
|
ALASM
|
||
2024-T3 |
28.60 - 36.10
|
1.876E+07
|
5.330E-08
|
NDT Mag
|
|
2024-T36 |
29.10 - 29.50
|
1.699E+07
|
5.884E-08
|
NDT Mag
|
|
2024-T3, T36, T351, T361, and T4 |
30.00
|
5.700E-08
|
ALASM
|
||
2024-T4 |
28.80 - 31.00
|
1.734E+07
|
5.766E-08
|
NDT Mag
|
|
2024-T6, T81, T851, and T861 |
38.00
|
4.500E-08
|
ALASM
|
||
2036-O |
52.00
|
3.320E-08
|
ALASM
|
||
2036-T4 |
41.00
|
4.210E-08
|
ALASM
|
||
2048-T851 |
42.00
|
4.000E-08
|
ALASM
|
||
2124-O |
50.00
|
3.450E-08
|
ALASM
|
||
2124-T851 |
39.00
|
4.421E-08
|
ALASM
|
resistivity converted from conductivity | |
2127-T4 |
42.10 - 42.40
|
2.451E+07
|
4.081E-08
|
NDT Mag
|
|
2218-T61 |
37.40
|
2.169E+07
|
4.610E-08
|
NDT Mag
|
|
2218-T61 |
38.00
|
4.500E-08
|
ALASM
|
||
2218-T72 |
40.00
|
4.300E-08
|
ALASM
|
||
2219-O |
44.00
|
3.900E-08
|
ALASM
|
||
2219-T31, T37, and T351 |
28.00
|
6.200E-08
|
ALASM
|
||
2219-T62, T81, T87, and T851 |
30.00
|
5.700E-08
|
ALASM
|
||
2319-O |
44.00
|
3.900E-08
|
ALASM
|
||
2618 |
40.20
|
2.332E+07
|
4.289E-08
|
NDT Mag
|
|
2618-T61 |
37.00
|
4.700E-08
|
ALASM
|
||
3003-O |
44.70 - 49.80
|
2.741E+07
|
3.649E-08
|
NDT Mag
|
|
3003-O |
50.00
|
3.400E-08
|
ALASM
|
||
3003-H14 and -H12 |
37.80 - 51.50
|
2.590E+07
|
3.861E-08
|
NDT Mag
|
|
3003-H12 |
42.00
|
4.100E-08
|
ALASM
|
||
3003-H14 |
41.00
|
4.200E-08
|
ALASM
|
||
3003-H18 |
40.00
|
4.300E-08
|
ALASM
|
||
3003-H24 and -H28 |
37.80 - 47.50
|
2.474E+07
|
4.043E-08
|
NDT Mag
|
|
3004 |
39.40 - 43.50
|
2.404E+07
|
4.160E-08
|
NDT Mag
|
|
3004-O |
42.00
|
4.100E-08
|
ALASM
|
||
X3005-O |
50.10 - 50.30
|
2.912E+07
|
3.435E-08
|
NDT Mag
|
|
3105-O |
45.00
|
3.830E-08
|
ALASM
|
||
4032-O |
40.00
|
4.310E-08
|
ALASM
|
||
4032-T6 |
35.30 - 36.30
|
2.076E+07
|
4.816E-08
|
NDT Mag
|
|
4032-T6 |
36.00
|
4.790E-08
|
ALASM
|
||
4043-F |
52.30 - 54.30
|
3.091E+07
|
3.235E-08
|
NDT Mag
|
|
4043-O |
42.00
|
4.100E-08
|
ALASM
|
||
5005 |
52.30 - 52.80
|
3.048E+07
|
3.281E-08
|
NDT Mag
|
|
5005-O and H38 |
52.00
|
3.320E-08
|
ALASM
|
||
5050 |
48.30 - 49.80
|
2.845E+07
|
3.515E-08
|
NDT Mag
|
|
5050-O and H38 |
50.00
|
3.400E-08
|
ALASM
|
||
5052 |
33.60 - 37.60
|
2.065E+07
|
4.843E-08
|
NDT Mag
|
|
5052-O and H38 |
35.00
|
4.930E-08
|
ALASM
|
||
5056 |
28.10 - 29.80
|
1.679E+07
|
5.956E-08
|
NDT Mag
|
|
5056-O |
29.00
|
5.900E-08
|
ALASM
|
||
5056-H38 |
27.00
|
6.400E-08
|
ALASM
|
||
5083 |
29.00
|
5.950E-08
|
ALASM
|
||
5086 |
31.00
|
5.600E-08
|
ALASM
|
||
5154 |
30.50 - 32.80
|
1.836E+07
|
5.448E-08
|
NDT Mag
|
|
5154 |
32.00
|
5.390E-08
|
ALASM
|
||
5182 |
31.00
|
5.560E-08
|
ALASM
|
||
5252 |
35.00
|
4.900E-08
|
ALASM
|
||
5254 |
32.00
|
5.400E-08
|
ALASM
|
||
5356-O |
29.00
|
5.940E-08
|
ALASM
|
||
5357 |
42.30 - 47.00
|
2.590E+07
|
3.861E-08
|
NDT Mag
|
|
5454 |
34.00
|
5.100E-08
|
ALASM
|
||
5456 |
29.00
|
5.950E-08
|
ALASM
|
||
5457 |
46.00
|
3.750E-08
|
ALASM
|
||
5652 |
35.00
|
4.900E-08
|
ALASM
|
||
5657 |
54.00
|
3.200E-08
|
ALASM
|
||
6005-T5 |
49.00
|
3.500E-08
|
ALASM
|
||
6009-O |
54.00
|
3.190E-08
|
ALASM
|
||
6009-T4 |
44.00
|
3.920E-08
|
ALASM
|
||
6009-T6 |
47.00
|
3.670E-08
|
ALASM
|
||
6010-O |
53.00
|
3.250E-08
|
ALASM
|
||
6010-T4 |
39.00
|
4.420E-08
|
ALASM
|
||
6010-T6 |
44.00
|
3.920E-08
|
ALASM
|
||
6053 |
39.30 - 48.00
|
2.532E+07
|
3.950E-08
|
NDT Mag
|
|
6061-F and -0 |
42.30 - 48.50
|
2.633E+07
|
3.798E-08
|
NDT Mag
|
|
6061-O |
47.00
|
3.700E-08
|
ALASM
|
||
6061-T4 |
37.60 - 40.50
|
2.265E+07
|
4.415E-08
|
NDT Mag
|
|
6061-T4 |
40.00
|
4.300E-08
|
ALASM
|
||
6061-T6 and -T9 |
40.00 - 44.80
|
2.459E+07
|
4.066E-08
|
NDT Mag
|
|
6061-T6 |
43.00
|
4.000E-08
|
ALASM
|
||
6062-F |
47.00 - 51.00
|
2.842E+07
|
3.519E-08
|
NDT Mag
|
|
6062-T4 |
43.50 - 44.00
|
2.538E+07
|
3.941E-08
|
NDT Mag
|
|
6062-T6 |
44.70 - 49.50
|
2.732E+07
|
3.661E-08
|
NDT Mag
|
|
6063-O |
58.00
|
3.000E-08
|
ALASM
|
||
6063-T1 |
50.00
|
3.500E-08
|
ALASM
|
||
6063-T5 |
55.00
|
3.200E-08
|
ALASM
|
||
6063-T6 and T83 |
53.00
|
3.300E-08
|
ALASM
|
||
6066-O |
40.00
|
4.300E-08
|
ALASM
|
||
6066-T6 |
37.00
|
4.700E-08
|
ALASM
|
||
6070-T6 |
44.00
|
3.900E-08
|
ALASM
|
||
6101-T6 |
57.00
|
3.020E-08
|
ALASM
|
||
6101-T61 |
59.00
|
2.920E-08
|
ALASM
|
||
6101-T63 |
58.00
|
2.970E-08
|
ALASM
|
||
6101-T64 |
60.00
|
2.870E-08
|
ALASM
|
||
6101-T65 |
58.00
|
2.970E-08
|
ALASM
|
||
6151-0 |
53.30 - 55.00
|
3.141E+07
|
3.184E-08
|
NDT Mag
|
|
6151-O |
54.00
|
3.200E-08
|
ALASM
|
||
6151-T4 |
41.50 - 43.30
|
2.459E+07
|
4.066E-08
|
NDT Mag
|
|
6151-T6 |
42.00
|
4.100E-08
|
ALASM
|
||
6151-T6 |
43.90 - 45.00
|
2.578E+07
|
3.879E-08
|
NDT Mag
|
|
6151-T6 |
45.00
|
3.800E-08
|
ALASM
|
||
6201-T81 |
54.00
|
3.200E-08
|
ALASM
|
||
6205-T1 |
45.00
|
3.700E-08
|
ALASM
|
||
6205-T5 |
49.00
|
3.500E-08
|
ALASM
|
||
6262-T9 |
44.00
|
3.900E-08
|
ALASM
|
||
6351-T6 |
46.00
|
3.800E-08
|
ALASM
|
||
6463-T1 |
50.00
|
3.400E-08
|
ALASM
|
||
6463-T5 |
55.00
|
3.100E-08
|
ALASM
|
||
6463-T6 |
53.00
|
3.300E-08
|
ALASM
|
||
6951-F |
53.00 - 53.10
|
3.077E+07
|
3.250E-08
|
NDT Mag
|
|
6951-0 |
55.70 - 56.50
|
3.254E+07
|
3.073E-08
|
NDT Mag
|
|
7005-O |
43.00
|
4.010E-08
|
ALASM
|
||
7005-T53, T5351, T63, and T6351 |
38.00
|
4.540E-08
|
ALASM
|
||
7005-T6 |
35.00
|
4.930E-08
|
ALASM
|
||
7039 |
32-40
|
4.3E-8--5.4E-8
|
ALASM
|
resistivity converted from conductivity | |
7049 |
40.00
|
4.300E-08
|
ALASM
|
||
7050-O |
47.00
|
3.670E-08
|
ALASM
|
||
7050-T76 and T7651 |
39.50
|
4.360E-08
|
ALASM
|
||
7050-T736 and T73651 |
40.50
|
4.260E-08
|
ALASM
|
||
7072 |
60.00 - 60.10
|
3.483E+07
|
2.871E-08
|
NDT Mag
|
|
7072-O |
60.00
|
2.870E-08
|
ALASM
|
||
7075-F |
44.50 - 47.80
|
2.677E+07
|
3.736E-08
|
NDT Mag
|
|
7075-T6 |
31.40 - 34.80
|
1.920E+07
|
5.209E-08
|
NDT Mag
|
|
7075-T6 |
32.00
|
1.856E+07
|
5.388E-08
|
ECTM
|
|
7075-W |
27.00 - 37.00
|
1.856E+07
|
5.388E-08
|
NDT Mag
|
|
7075-T6, T62, T651, and T652 |
33.00
|
5.220E-08
|
ALASM
|
||
7075-T76 and T7651 |
38.50
|
4.480E-08
|
ALASM
|
||
7075-T73, T7351, and T7352 |
40.00
|
4.310E-08
|
ALASM
|
||
7076 |
35.00
|
3.750E-08
|
ALASM
|
||
7175-O |
46.00
|
3.750E-08
|
ALASM
|
||
7175-T66 |
36.00
|
4.790E-08
|
ALASM
|
||
7175-T736 and T73652 |
40.00
|
4.310E-08
|
ALASM
|
||
7178-O |
46.00
|
3.750E-08
|
ALASM
|
||
7178-T6 and T651 |
32.00
|
5.390E-08
|
ALASM
|
||
7178-T76 and T7651 |
39.00
|
4.420E-08
|
ALASM
|
||
X7178-F and -0 |
45.50 - 46.00
|
2.654E+07
|
3.769E-08
|
NDT Mag
|
|
X7178-W and T6 |
26.80 - 32.60
|
1.723E+07
|
5.805E-08
|
NDT Mag
|
|
7475-O |
46.00
|
3.750E-08
|
ALASM
|
||
7475-T61 and T651 |
36.00
|
4.790E-08
|
ALASM
|
||
7475-T761 and T7651 |
40.00
|
4.310E-08
|
ALASM
|
||
7475-T7351 |
42.00
|
4.110E-08
|
ALASM
|
||
|
|
|
|
||
Aluminum Alloys (Cast) |
|||||
122 Perm. Mold As Cast |
34.00
|
1.972E+07
|
5.071E-08
|
CSNDT
|
|
122 Sand Cond. T2 |
41.00
|
2.378E+07
|
4.205E-08
|
CSNDT
|
|
122 Sand Cond. T61 |
33.00
|
1.914E+07
|
5.225E-08
|
CSNDT
|
|
113 |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
C113 |
27.00
|
1.566E+07
|
6.386E-08
|
CSNDT
|
|
A 132 Cond. T551 |
29.00
|
1.682E+07
|
5.945E-08
|
CSNDT
|
|
201.0-T6 |
27-32
|
4.5E-8--6.4E-8
|
ALASM
|
||
206.0-T6 |
27-32
|
5.4E-8--6.4E-8
|
ALASM
|
conductivity converted from resistivity | |
206.0-T7 |
32-34
|
5.0E-8--5.4E-8
|
ALASM
|
conductivity converted from resistivity | |
208.0 as-cast |
31.00
|
5.560E-08
|
ALASM
|
||
(208.0) 108 |
31.00
|
1.798E+07
|
5.562E-08
|
CSNDT
|
|
208.0 annealed |
38.00
|
4.540E-08
|
ALASM
|
||
214 |
35.00
|
2.030E+07
|
4.926E-08
|
CSNDT
|
|
A214 |
33.00
|
1.914E+07
|
5.225E-08
|
CSNDT
|
|
218 |
24.00
|
1.392E+07
|
7.184E-08
|
CSNDT
|
|
220 |
21.00
|
1.218E+07
|
8.210E-08
|
CSNDT
|
|
242.0-T21, sand |
44.00
|
3.920E-08
|
ALASM
|
||
(242.0) 142 Sand Cond. T21 |
44.00
|
2.552E+07
|
3.918E-08
|
CSNDT
|
|
242.0-T571, sand |
34.00
|
5.070E-08
|
ALASM
|
||
(242.0) 142 Sand Cond. T571 |
34.00
|
1.972E+07
|
5.071E-08
|
CSNDT
|
|
242.0-T77, sand |
38.00
|
4.540E-08
|
ALASM
|
||
(242.0) 142 Sand Cond. T77 |
37.00
|
2.146E+07
|
4.660E-08
|
CSNDT
|
|
242.0-T61, permanent mold |
33.00
|
5.220E-08
|
ALASM
|
||
295.0-T4 |
35.00
|
4.930E-08
|
ALASM
|
||
(295.0) 195 Cond. T4 |
35.00
|
2.030E+07
|
4.926E-08
|
CSNDT
|
|
295.0-T62 |
37.00
|
4.930E-08
|
ALASM
|
||
(295.0) 195 Cond. T62 |
37.00
|
2.146E+07
|
4.660E-08
|
CSNDT
|
|
296.0-T4 and T6 |
33.00
|
5.220E-08
|
ALASM
|
||
(296.0) B 195 Cond. T4 |
35.00
|
2.030E+07
|
4.926E-08
|
CSNDT
|
|
(296.0) B 195 Cond. T6 |
36.00
|
2.088E+07
|
4.789E-08
|
CSNDT
|
|
308.0 |
37.00
|
4.660E-08
|
ALASM
|
||
(308.0) A 108 |
37.00
|
2.146E+07
|
4.660E-08
|
CSNDT
|
|
R 317 |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
319.0 |
27.00
|
6.390E-08
|
ALASM
|
||
319 Sand |
27.00
|
1.566E+07
|
6.386E-08
|
CSNDT
|
|
319 Perm. Mold |
28.00
|
1.624E+07
|
6.158E-08
|
CSNDT
|
|
336.0-T551 |
29.00
|
5.950E-08
|
ALASM
|
||
355.0-T51, sand |
43.00
|
4.010E-08
|
ALASM
|
||
355 Sand Cond. T51 |
43.00
|
2.494E+07
|
4.010E-08
|
CSNDT
|
|
355.0-T6, sand |
36.00
|
4.790E-08
|
ALASM
|
||
355 Sand Cond. T6 |
36.00
|
2.088E+07
|
4.789E-08
|
CSNDT
|
|
355.0-T61, sand |
39.00
|
4.420E-08
|
ALASM
|
||
355 Sand Cond. T61 |
37.00
|
2.146E+07
|
4.660E-08
|
CSNDT
|
|
355.0-T7, sand |
42.00
|
4.100E-08
|
ALASM
|
||
355 Sand Cond. T7 |
42.00
|
2.436E+07
|
4.105E-08
|
CSNDT
|
|
355.0-T6, permanent mold |
39.00
|
4.420E-08
|
ALASM
|
||
355 Perm. Mold Cond. T6 |
39.00
|
2.262E+07
|
4.421E-08
|
CSNDT
|
|
356.0-T51, sand |
43.00
|
4.010E-08
|
ALASM
|
||
356 Sand Cond. T51 |
43.00
|
2.494E+07
|
4.010E-08
|
CSNDT
|
|
356.0-T6, sand |
39.00
|
4.420E-08
|
ALASM
|
||
356 Sand Cond. T6 |
39.00
|
2.262E+07
|
4.421E-08
|
CSNDT
|
|
356.0-T7, sand |
40.00
|
4.310E-08
|
ALASM
|
||
356.0-T6, permanent mold |
41.00
|
4.210E-08
|
ALASM
|
||
360.0 |
28.00
|
6.160E-08
|
ALASM
|
||
A360.0 |
30.00
|
5.747E-08
|
ALASM
|
resistivity converted from conductivity | |
360 |
37.00
|
2.146E+07
|
4.660E-08
|
CSNDT
|
|
380.0 |
27.00
|
6.500E-08
|
ALASM
|
||
380 |
27.00
|
1.566E+07
|
6.386E-08
|
CSNDT
|
|
383.0 |
23.00
|
7.496E-08
|
ALASM
|
resistivity converted from conductivity | |
384.0 |
22.00
|
7.837E-08
|
ALASM
|
resistivity converted from conductivity | |
A384.0 |
23.00
|
7.496E-08
|
ALASM
|
resistivity converted from conductivity | |
390.0-F |
27.00
|
6.386E-08
|
ALASM
|
resistivity converted from conductivity | |
390.0-T5 |
25.00
|
6.896E-08
|
ALASM
|
resistivity converted from conductivity | |
413.0 |
31.00
|
5.56E-08
|
ALASM
|
||
443.0 As-Cast |
37.00
|
4.660E-08
|
ALASM
|
||
443.0 Annealed |
42.05
|
4.100E-08
|
ALASM
|
conductivity converted from resistivity | |
514.0 |
35.00
|
4.930E-08
|
ALASM
|
||
518.0 |
25.00
|
6.896E-08
|
ALASM
|
resistivity converted from conductivity | |
520.0-T4 |
21.00
|
8.210E-08
|
ALASM
|
||
535.0 |
20.00
|
7.500E-08
|
ALASM
|
||
712.0 |
35.00
|
4.930E-08
|
ALASM
|
||
713.0 |
35.00
|
4.926E-08
|
ALASM
|
resistivity converted from conductivity | |
750 |
45.00
|
2.610E+07
|
3.831E-08
|
CSNDT
|
|
771.0 |
27.00
|
6.386E-08
|
ALASM
|
resistivity converted from conductivity | |
850.0 |
47.00
|
3.670E-08
|
ALASM
|
- ALASM=ASM Specialty Handbook Aluminum and Aluminum Alloys
- CSNDT=CSNDT compiled by Eddy Current Technology Incorporated
- ECTM=Eddy Current Testing Manual on Eddy Current Melted compiled by Eddy Current Technology Incorporated
- NDT Mag=NDT Magazine Sept/Oct 1955, Cosgrove Article compiled by Eddy Current Technology Incorporated
Compiled by the Collaboration for NDT Education